Sacrificial anode - what to expect

Hello fellow TFers.
Last week my boat was hauled out and yesterday I went to empty it for winter.
Before splashing in may I replaced all the anodes with new ones and added few where the previous owner was not looking.
My question is what wear to expect after 6 month?
I was a bit surprised by the level of wear as I found them well marked from dissolution.
I will take a picture next weekend to illustrate this.
I may worry for nothing but it is the first time I install new anodes.

L
Lou_tribal is offline   Reply With Quote
Old 10-15-2017, 06:04 PM   #2
Valued Technical Contributor
 
DavidM's Avatar
 
City: Litchfield, Ct
Join Date: Aug 2012
Posts: 6,786
Hull anodes usually last a year or more before needing replacement. If yours are going before that, it may be due to an electrical problem in your boat or an adjacent boat at your marina.

David
DavidM is offline   Reply With Quote
Old 10-15-2017, 06:10 PM   #3
Guru
 
Lou_tribal's Avatar
 
City: Quebec
Vessel Name: Bleuvet
Vessel Model: Custom Built
Join Date: Jan 2016
Posts: 4,375
Quote:
Originally Posted by djmarchand View Post
Hull anodes usually last a year or more before needing replacement. If yours are going before that, it may be due to an electrical problem in your boat or an adjacent boat at your marina.

David


Ok if they should last 1 year I guess mine are fine. I was not expecting such a wear!
I am in fresh water and my anode are magnesium.
For the two round ones on the rudder I can see that they decreased by something like 1/8th of an inch. Was not thinking it was so much.
A question from some green wood captain lol

L
Lou_tribal is offline   Reply With Quote
Old 10-15-2017, 06:12 PM   #4
Guru
 
City: Great Lakes
Vessel Model: OA 440
Join Date: Aug 2017
Posts: 906
I just purchased a new set for our Great Lakes/fresh water boat. Switched from zinc to magnesium. Expecting to see increased "erosion".
Rufus is offline   Reply With Quote
Old 10-15-2017, 07:18 PM   #5
Guru
 
C lectric's Avatar
 
City: Gibsons, B.C., Canada
Vessel Name: Island Pride
Vessel Model: Palmer 32'
Join Date: Oct 2007
Posts: 4,414
Your anode use sounds about right especially for magnesium. Better it is being used than not. If you are not happy with the time they last then either add bigger ones or another anode or two.

Just do not go overboard [??] on them. Even on fiberglass boats there can be some odd effects if the zincing is really overboard. .

Dave Gerr has published some ways to calculate, roughly, how much zinc is needed for some applications.
C lectric is offline   Reply With Quote
Old 10-15-2017, 07:32 PM   #6
Guru
 
BandB's Avatar
 
City: Fort Lauderdale. Florida, USA
Join Date: Jan 2014
Posts: 21,449
Quote:
Originally Posted by Lou_tribal View Post
Ok if they should last 1 year I guess mine are fine. I was not expecting such a wear!
I am in fresh water and my anode are magnesium.
For the two round ones on the rudder I can see that they decreased by something like 1/8th of an inch. Was not thinking it was so much.
A question from some green wood captain lol

L
Magnesium has a much shorter life than zinc or aluminum. Of course Zinc isn't appropriate for fresh water. We use aluminum.

Boat zincs has charts, Chart A and B, that you can reach from this page to help in your selection. Also a table showing a comparison by material.

BoatZincs.com (978-841-9978) - FAQs
BandB is offline   Reply With Quote
Old 10-15-2017, 07:46 PM   #7
Guru
 
Lou_tribal's Avatar
 
City: Quebec
Vessel Name: Bleuvet
Vessel Model: Custom Built
Join Date: Jan 2016
Posts: 4,375
Thank you all, as it was the first time I was checking anode from new set I was not sure about what to expect. As mentioned I was thinking that if they look dissolved it was a good clue that there were working as expected but in the same time I was worrying that if they are too much dissolved something was wrong. I guess I am thinking and worrying too much

L
Lou_tribal is offline   Reply With Quote
Old 10-15-2017, 08:24 PM   #8
Moderator Emeritus
 
Comodave's Avatar
 
City: Au Gres, MI
Vessel Name: Black Dog
Vessel Model: Formula 41PC
Join Date: Jul 2015
Posts: 21,191
Generally if they are half gone you should replace them. When we had a boat in southern California we would get about 6 months or so from actual zincs since it was salt water. We just hauled our boat in Michigan which I had installed aluminum anodes on this spring. Although they are not half gone, I will change them over the winter so I don't have to change them during the summer next year. With the erosion that has occurred this year I don't think they will last another season and not go below the halfway mark.
Comodave is online now   Reply With Quote
Old 10-15-2017, 08:29 PM   #9
Guru
 
Ken E.'s Avatar
 
City: Bellingham WA
Vessel Name: Hatt Trick
Vessel Model: 45' Hatteras Convertible
Join Date: Nov 2016
Posts: 1,973
Quote:
Originally Posted by C lectric View Post
Your anode use sounds about right especially for magnesium. Better it is being used than not. If you are not happy with the time they last then either add bigger ones or another anode or two.

Just do not go overboard [??] on them. Even on fiberglass boats there can be some odd effects if the zincing is really overboard. .

Dave Gerr has published some ways to calculate, roughly, how much zinc is needed for some applications.
Clark, I don't think I'm getting enough zinc wear, meaning they may not be doing their job. I have two transom plates that are two years old and they're pitted, but they look like they could go easily for another year. I have an isolation transformer which may be part of the explanation.

The boat is presently on the hard. What I intend to do is put a meter between the zincs and underwater metal and look for .5 ohms. Is this in the ball park?

Also, how can I get at the Dave Gerr data? Is it at this site?
____________________
Ken Hatt Trick
Ken E. is offline   Reply With Quote
Old 10-15-2017, 10:51 PM   #10
Guru
 
C lectric's Avatar
 
City: Gibsons, B.C., Canada
Vessel Name: Island Pride
Vessel Model: Palmer 32'
Join Date: Oct 2007
Posts: 4,414
Re: Dave Gerr. You might try googling for the info. about it. I haven't looked but I would guess other sources would be available. If need be I could try scanning the pages.

0.5 ohm between the zinc plates and the metals would be a good figure. Most meters have trouble getting reliable readings past that unless it's a highly specialized meter which is not needed for this. Generally I look for less than 1 ohm.
Check the meter probes themselves and clean them as any oxidation can affect readings at that level. Clean a spot on the zinc and on the metal you are checking. Then use the meter.

Yes, an isolation transformer will reduce the likely hood of zinc wastage from leaking A.C.

If the plates are large enough that may be why you don't see a faster zinc wastage. Large zincs compared to the metals protected, no leakage either from your boat or others, and the result may be what you are experiencing.

If the ohm reading is on the high side then check the zinc mounts themselves. Some times the zinc wastage can affect the actual mounting area. If so then a good cleaning may be in order to restore the mounting area, both on the zinc and the pad.

One of the best ways to check zinc action and the protection at each piece of equipment is the use of a silver/silver chloride half cell. They are available from Boatzincs.com and can be used with a dmm quite effectively.

I use one I bought a long time ago from Promariner as a kit, an analogue meter, and it has helped big time showing me a couple cases where the bonding had been lost.

All you should need is the cell from Boatzinc and a long ground lead with a large, heavy duty alligator clip along with your DMM. At the time I bought mine I was too ignorant of what was available and I don't think folk like Boatzinc was around.
I like my meter but now I would simply get the cell.
C lectric is offline   Reply With Quote
Old 10-15-2017, 10:53 PM   #11
Guru
 
tiltrider1's Avatar
 
City: Seattle
Vessel Name: AZZURRA
Vessel Model: Ocean Alexander 54
Join Date: Aug 2017
Posts: 4,309
If the boat is on the hard then perform a continuity check between your zinc plates and all your under water metal. Use a multi meter set to ohms and look for OL on the display.

If you have continuity you will have protection.
tiltrider1 is offline   Reply With Quote
Old 10-16-2017, 12:10 AM   #12
Master and Commander
 
markpierce's Avatar
 
City: Vallejo CA
Vessel Name: Carquinez Coot
Vessel Model: penultimate Seahorse Marine Coot hull #6
Join Date: Sep 2010
Posts: 12,559
By definition, they are sacrificial. I get by with annual inspections, and as-needed, replacements.
__________________
Kar-KEEN-ez Koot
markpierce is offline   Reply With Quote
Old 10-16-2017, 05:17 PM   #13
Guru
 
kchace's Avatar
 
City: Brookline, NH
Vessel Name: Shalloway
Vessel Model: Defever 44, twin Perkins
Join Date: Sep 2013
Posts: 2,260
I've gone to aluminum but with 4 shaft "zincs" one on each rudder and 2 on the transom, they are about 50% wasted after 6 months.

Ken
kchace is offline   Reply With Quote
Old 10-19-2017, 08:13 AM   #14
Guru
 
foggysail's Avatar
 
City: Ashland, MA
Vessel Model: 1990 Silverton 40 aftcabin
Join Date: Jul 2016
Posts: 1,208
The amount of surface area of exposed metals, types of metals to be protected along with the water conductivity are going to determine the anode life.
foggysail is offline   Reply With Quote
Old 10-24-2017, 07:58 PM   #15
Guru
 
foggysail's Avatar
 
City: Ashland, MA
Vessel Model: 1990 Silverton 40 aftcabin
Join Date: Jul 2016
Posts: 1,208
Quote:
Originally Posted by foggysail View Post
The amount of surface area of exposed metals, types of metals to be protected along with the water conductivity are going to determine the anode life.


We put our boat to rest yesterday until spring. Prior to hauling, I tested my anode's performance. SOLID! My measured voltages on all metals including my shafts which are bonded via my custom made (by me) shaft brushes were in the -0.78 range. The readings matched those taken back in May when we launched.

My single anode is a stern mounted aluminum 6 X 12 X 1" diver's plate style. Last year's test of my anode performance prior to haul caused concern when I saw my galvanic protection starting to fail. Sure enough, after hauling I found my anode almost completely disintegrated. So this year I purchased one that is 1" thick instead of 1/2" thick.
foggysail is offline   Reply With Quote
Old 02-03-2018, 05:48 PM   #16
Guru
 
Lou_tribal's Avatar
 
City: Quebec
Vessel Name: Bleuvet
Vessel Model: Custom Built
Join Date: Jan 2016
Posts: 4,375
Ok after few weeks (months) here are the pictures of my anodes after 1 season. They were put in new in may 2017 and pictures were taken end of October 2017. What do you think about it? (On the blury shaft pic the first anode is the new one, the second is an old zinc one I left there)
Note: they are all zinc.

Click image for larger version

Name:	20171021_142312.jpg
Views:	87
Size:	130.4 KB
ID:	72664Click image for larger version

Name:	20171021_142306.jpg
Views:	87
Size:	76.2 KB
ID:	72665Click image for larger version

Name:	20171021_142303.jpg
Views:	91
Size:	100.8 KB
ID:	72666Click image for larger version

Name:	20171021_142136.jpg
Views:	93
Size:	71.3 KB
ID:	72667
Lou_tribal is offline   Reply With Quote
Old 02-03-2018, 05:52 PM   #17
Guru
 
BruceK's Avatar
 
City: Sydney
Vessel Name: Sojourn
Vessel Model: Integrity 386
Join Date: Oct 2011
Posts: 13,333
Very disappointing Lou. They need polishing, what must the fish think.
__________________
BruceK
2005 Integrity 386 "Sojourn"
Sydney Australia
BruceK is offline   Reply With Quote
Old 02-03-2018, 06:00 PM   #18
Moderator Emeritus
 
Comodave's Avatar
 
City: Au Gres, MI
Vessel Name: Black Dog
Vessel Model: Formula 41PC
Join Date: Jul 2015
Posts: 21,191
Lou,

Is your boat in salt water? In one of the preceding you said the anodes were magnesium and now you said they are zinc. In freash water they should be magnesium or aluminum. Why did you leave the old anode on your shaft in addition to the new one?
Comodave is online now   Reply With Quote
Old 02-03-2018, 06:13 PM   #19
Guru
 
Lou_tribal's Avatar
 
City: Quebec
Vessel Name: Bleuvet
Vessel Model: Custom Built
Join Date: Jan 2016
Posts: 4,375
Quote:
Originally Posted by BruceK View Post
Very disappointing Lou. They need polishing, what must the fish think.
Yeah I know I am leasy, I should sand and varnish them

L
Lou_tribal is offline   Reply With Quote
Old 02-03-2018, 06:17 PM   #20
Guru
 
Lou_tribal's Avatar
 
City: Quebec
Vessel Name: Bleuvet
Vessel Model: Custom Built
Join Date: Jan 2016
Posts: 4,375
Quote:
Originally Posted by Comodave View Post
Lou,

Is your boat in salt water? In one of the preceding you said the anodes were magnesium and now you said they are zinc. In freash water they should be magnesium or aluminum. Why did you leave the old anode on your shaft in addition to the new one?
My boat is in fresh water. The anode I installed are magnesium. The one that is zinc is an old one on the shaft (the background most on the pic). I kept it there as the bolts were stuck and was thinking it would not make any damage to keep it. The old one was installed by the PO who was not caring much about anodes.

L
Lou_tribal is offline   Reply With Quote
Reply

Thread Tools Search this Thread
Search this Thread:

Advanced Search
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Trackbacks are Off
Pingbacks are Off
Refbacks are Off


» Trawler Port Captains
Port Captains are TF volunteers who can serve as local guides or assist with local arrangements and information. Search below to locate Port Captains near your destination. To learn more about this program read here: TF Port Captain Program





All times are GMT -5. The time now is 03:35 AM.


Powered by vBulletin® Version 3.8.8 Beta 4
Copyright ©2000 - 2024, vBulletin Solutions, Inc.
Search Engine Optimization by vBSEO 3.6.0
Copyright 2006 - 2012